Introduction
A PET film line can lose intrinsic viscosity (IV) in a single extrusion pass. A different film may leave the line within specification and split only after warm, humid storage. These failures call for different corrective actions. Sampling the resin at the feed throat, the film at release and the same film after ageing shows where the loss starts.
What a drop in IV tells you
Water cleaves the ester linkage between a terephthalate-derived carbonyl and the ethylene glycol-derived segment. The resulting shorter chains typically lower IV. Compare IV alongside feed moisture and processing history. Excessive thermal exposure can also reduce IV, so a low value alone does not establish hydrolysis. For recycled PET, characterize each feedstock lot before attributing the loss to extrusion.
Figure 1. PET hydrolysis and carbodiimide stabilization
1. Ester-bond cleavage
P–C(=O)–O–CH₂CH₂–O–P + H₂O → P–COOH + HO–CH₂CH₂–O–P
2. Capture of the carboxyl end group
P–COOH + R¹–N=C=N–R² → O-acylisourea intermediate → N-acylurea adduct
Where PET film is most sensitive
For clear functional film, gels, haze and yellowing can rule out a formulation even if IV improves. For industrial sheet or film used in warm, humid environments, track tensile elongation and fracture behavior after exposure. Specify the resin blend ratio, film gauge and orientation because they affect comparisons between trials.
A practical selection guide
| Observed problem | What to check | What to evaluate first |
|---|---|---|
| IV falls between dried feed and finished film | Measure moisture at the hopper and check regrind handling and residence time. | Drying and process correction |
| IV is stable at release but elongation falls after ageing | Compare mechanical retention and IV against the dry-heat control. | HyMax® stabilization |
| Dry rPET starts below the target IV or gives weak melt strength | Check pressure, melt response, haze and gel count. | Discuss a KL-180 chain-extension trial |
How to qualify HyMax® and KL-180
A PET-compatible HyMax® masterbatch can simplify gravimetric dosing. Discuss M10 with Langyi for a PET carrier route and request the current specification, active content and let-down basis. For direct compounding, compare candidate forms against equipment capability and optical requirements.
Run a dried, additive-free control and a HyMax®-only formulation at supplier-recommended levels. Add a KL-180-only trial where a defined melt-processing issue warrants it. Record resin and additive lots, active content or let-down, drying and processing history. Compare both initial and aged results against a predefined acceptance threshold before deciding whether to try a combination.
Frequently asked questions
How much IV should we recover?
Set the target from the product specification and line window. Track gels, haze and melt pressure at the same time so viscosity recovery does not mask another failure.
Can a hydrolysis stabilizer replace resin drying?
Follow the resin supplier’s drying guidance and record moisture at the feed point. An additive trial is easier to interpret when every formulation starts from a comparable moisture history.
Discuss your application with Langyi
Share your resin grade, processing route, target properties and ageing conditions when contacting Hong Kong Langyi. See related applications in Polymers, Films & Coatings.